Hi all. I fix electronics for fun and from stubbornness, and the number one cause of "it worked yesterday" on old boards is a cold or cracked solder joint.
How to spot one: dull, grainy or lumpy surface instead of a bright, smooth cone; a visible gap or ring around the pin; a joint that moves when you press the part. Under magnification a ring crack around a through-hole pin looks like a tiny canyon.
How to avoid making one:
- Clean surfaces. Oxidised pads will not wet. A little isopropyl alcohol and a brush.
- Flux. Cored solder wire carries a little flux, but fresh flux on a rework joint makes a visible difference.
- Heat both parts: the pad and the lead at the same time, then feed the solder to the joint, not to the iron tip.
- Do not move the joint while it cools. Count to five.
- Right temperature. Lead-free solder melts higher than the old tin-lead alloy (typically around 217 C against 183 C), so it needs a hotter iron and more patience, and the joints look duller even when they are good. That is my annual rant, and I am keeping it short.
Fix for a suspect joint: add fresh flux, reheat, add a touch of new solder. Do not just "touch it up" with a cold iron.